    Electrochemical Characterization: Seven Essential Tests and Their Typical Curves

    This article introduces seven common battery tests: galvanostatic charge–discharge, rate capability, long-term cycling, cyclic voltammetry, linear sweep voltammetry, electrochemical impedance spectroscopy and galvanostatic intermittent titration. It explains what each method measures, how to interpret typical curves and which test conditions matter, helping readers select suitable methods to assess battery capacity, cycling stability, electrochemical reactions, impedance and ion transport within electrodes.

    Latest updated: November 24, 2026 Reading time: 8 - 10 min

    1 Galvanostatic charge–discharge reveals capacity and voltage profiles

    Galvanostatic charge–discharge (GCD) applies a constant current and records voltage until a cutoff condition is reached. Figure 1a shows the current input above the voltage response. Voltage is usually plotted against time or capacity: the endpoint on the horizontal axis indicates the charge passed under the test conditions, while plateaus and sloping regions describe the voltage profile of the reaction. Curve shape depends on the material; a flatter plateau does not necessarily indicate better performance. [1]

    Capacity during a constant-current step is calculated using the equation below, where Q is capacity, I is current and Δt is duration. If the protocol also includes a constant-voltage step, its charge contribution must be added separately. Sample comparisons require consistent current, cutoff voltage, temperature and capacity normalization. Specific capacity based on active-material mass must not be treated as the specific capacity of the complete cell.

    English Equation 01 Capacity

    Coulombic efficiency compares the charge passed during paired discharge and charge processes. Qdischarge and Qcharge denote the respective capacities. It differs from energy efficiency, which also accounts for voltage, and a high value in one cycle cannot establish long-term stability. [1]

    English Equation 02 Coulombic Efficiency

    GCD and GITT protocols

    Figure 1. Controlled variables and response curves for galvanostatic and potentiostatic methods

    Further reading: Charge–discharge steps and parameter settings (NEWARE)

    2 Rate capability testing compares performance at different currents

    Rate capability testing varies the charging or discharging current and measures capacity and voltage response. C-rate is calculated from a specified reference capacity: for a 2 Ah reference capacity, 1 C corresponds to 2 A, 0.5 C to 1 A and 2 C to 4 A. These values do not guarantee that actual charging or discharging will finish within the corresponding theoretical time. A protocol may progressively increase the discharge rate and then return to a lower rate; whether the charging conditions remain fixed should be stated. [1,9]

    Typical results include voltage–capacity curves at different rates and capacity plotted over successive rate stages. Higher current often lowers the discharge voltage and may cause the cutoff voltage to be reached before as much capacity is delivered. Capacity recovery after returning to a lower rate helps distinguish reversible rate limitations from possible irreversible changes, but does not by itself prove the absence of damage. Report reference capacity, temperature, charging and discharging strategy, and cutoff conditions when comparing rate capability.

    Rate performance data

    Figure 2. Specific capacity versus cycle number during rate capability testing

    Further reading: Battery rate performance and BTS step settings (NEWARE)

    3 Long-term cycling tracks performance over repeated cycles

    Long-term cycling repeats specified charging, discharging and rest steps while recording capacity, coulombic efficiency and other metrics. Typical plots show discharge capacity or capacity retention against cycle number. Capacity retention is the ratio of the current capacity to a selected reference capacity. The reference may be a specified initial cycle or a reference performance test; it must be stated clearly so that differences during activation are not mistaken for differences in degradation. [1,9]

    Look for the rate of capacity fade, any acceleration in the decline and variation among samples in the same batch. Cycle count is meaningful only alongside C-rate, temperature, depth of discharge and the end-of-life criterion; counts obtained under different conditions cannot be ranked directly. Reference capacity and internal-resistance measurements under consistent conditions can be inserted at specified intervals to help distinguish capacity loss from changes in polarization. [9]

    Cycle performance data

    Figure 3. Specific capacity and coulombic efficiency in the cycling data interface

    Further reading: How depth of discharge affects battery cycle life (NEWARE)

    4 Cyclic voltammetry reveals oxidation and reduction peaks

    Cyclic voltammetry (CV) sweeps potential forward and backward at a specified scan rate while recording current. Potential is plotted on the horizontal axis and current or current density on the vertical axis. Peak positions help identify reaction regions; peak shapes and separation between the forward and reverse scans provide clues about reversibility. Figure 4 is a theoretical example for an ideal reversible, diffusion-controlled system: peak current increases with scan rate while peak positions remain essentially unchanged. Its potential axis is referenced to the formal potential E°′, rather than the operating voltage of a battery. [2]

    CV scan rates

    Figure 4. Theoretical cyclic voltammograms at different scan rates

    Peak height also depends on scan rate, active-material loading and effective area, so it cannot be used directly to compare capacity. In practical battery electrodes, peak shifts or increased peak separation may reflect kinetic limitations, ohmic drop and other contributions. CV is useful for comparing reaction regions and changes before and after cycling under matching conditions. Reversibility criteria for ideal solution systems should not be applied directly to complex porous electrodes. [2,3]

    Further reading: Cyclic voltammetry principles and applications (NEWARE)

    5 Linear sweep voltammetry screens stability limits

    Linear sweep voltammetry (LSV) scans potential in one direction while recording current, often to identify the onset of electrolyte oxidation or reduction. Figure 5 shows the potential–time input on the left and the current response on the right. It illustrates the principle; its potential values do not define the stability window of a particular electrolyte. Identify the discernible reaction onset when assessing a stability limit, rather than simply taking the current peak. [4]

    LSV principle 

    Figure 5. Input signal and current response in linear sweep voltammetry

    An anodic scan usually provides information about the oxidative limit only; the reductive limit must also be assessed to establish a complete stability window. The working electrode, scan rate, temperature and current-onset criterion can all affect the result. LSV is useful for initial screening. A small current during a short scan does not establish the absence of long-term side reactions, so potentiostatic holds or cycling tests with the relevant electrodes are also needed. [4,5]

    Further reading: Linear voltammetry principles and curve analysis (NEWARE)

    6 EIS measures impedance responses across frequency

    Electrochemical impedance spectroscopy (EIS) applies a small alternating perturbation around a selected operating state and varies its frequency to obtain amplitude and phase information. A Nyquist plot usually displays the real impedance Z′ on the horizontal axis and the negative imaginary component −Z″ on the vertical axis, with each point corresponding to one frequency. Bode plots directly show impedance magnitude and phase versus frequency. Figures 6b and 6c present these two representations of the same measurement data. [1,6]

    In typical battery spectra, the high-frequency region may include ohmic and fast conduction responses, arcs may involve interfacial and charge-transfer processes, and the low-frequency tail is often associated with mass transport or diffusion. These processes can overlap, and their frequency ranges change with cell state. Equivalent-circuit fitting provides model parameters; a constant phase element (CPE) represents a non-ideal capacitive response. EIS helps examine contributions to impedance changes, but a single semicircle or a good fit does not uniquely identify a degradation mechanism. [1,6]

    EIS principle and spectra

    Figure 6. EIS excitation and response, Bode and Nyquist plots, and an equivalent circuit

    Further reading: EIS principles and spectrum analysis (NEWARE)

    7 GITT analyzes voltage relaxation after current pulses

    The galvanostatic intermittent titration technique (GITT) divides charging or discharging into short constant-current steps separated by zero-current rest periods, as shown in Figure 1c. Look for the rapid voltage change at current onset, the continued change during the pulse and the slower recovery after current interruption. Sufficiently relaxed endpoints can describe a quasi-open-circuit voltage curve. An endpoint that is still changing appreciably should not be treated as an equilibrium potential. [1,7]

    Under suitable model assumptions, GITT can estimate an apparent chemical diffusion coefficient and its variation with lithiation state. Pulse duration, effective area, particle geometry, two-phase transitions and treatment of rapid voltage drops all affect the result. In a commercial full cell, multiple processes in both electrodes contribute to the voltage response; their individual diffusion coefficients cannot be obtained separately from the full-cell curve alone. [7]

    GITT pulse and diffusivity

    Figure 7. From GITT charge–discharge curves to diffusion coefficients

    Read Figure 7 in the order a → b → c → d,e: start with the pulsed charge–discharge curves, enlarge one pulse–rest sequence, and extract the pulse duration τ, the voltage change during the pulse after excluding the instantaneous ohmic drop (ΔEτ), and the difference between the fully relaxed potentials before and after the pulse (ΔEs). This study used 0.1 C pulses lasting 0.5 h, followed by 2 h rest periods; these are the conditions of that particular experiment. [10]

    Where the short-time diffusion assumptions hold and potential is approximately linear in √t, the diffusion coefficient can be estimated using Equation (3). Va is the volume of active material participating in the reaction and S is the effective reaction area. Calculating a value for each pulse and associating it with the corresponding potential produces curves such as Figures 7d and 7e. Figure 7f is an independent EIS comparison and is not used in this calculation. [7,10]

    English Equation 03 GITT Diffusivity

    Video tutorial: Copying GITT data and graphs (NEWARE)

    Further reading: GITT diffusivity measurements: assumptions and error sources (NEWARE)

    Selecting methods and equipment for the measurement objective

    Capacity, rate capability and long-term cycling address basic battery performance. CV identifies reaction regions, while LSV screens stability limits. EIS examines frequency-dependent impedance responses, and GITT adds relaxation and diffusion analysis. When combining methods, keep temperature, state of charge (SOC) and electrode configuration comparable; curves measured under different conditions should not be combined directly into a mechanistic conclusion.

    NEWARE can support testing in these areas. Please contact customer service to discuss your specific testing requirements.

    References

    [1] Ugata, Y.; Motoki, C.; Dokko, K.; Yabuuchi, N. Fundamental methods of electrochemical characterization of Li insertion materials for battery researchers. Journal of Solid State Electrochemistry 28, 1387–1401 (2024). 

    [2] Yamada, H.; Yoshii, K.; Asahi, M.; Chiku, M.; Kitazumi, Y. Cyclic Voltammetry Part 1: Fundamentals. Electrochemistry 90(10), 102005 (2022).

    [3] Espinoza, E. M.; Clark, J. A.; Soliman, J.; Derr, J. B.; Morales, M.; Vullev, V. I. Practical Aspects of Cyclic Voltammetry: How to Estimate Reduction Potentials When Irreversibility Prevails. Journal of The Electrochemical Society 166(5), H3175–H3187 (2019). 

    [4] Méry, A.; Rousselot, S.; Lepage, D.; Dollé, M. A Critical Review for an Accurate Electrochemical Stability Window Measurement of Solid Polymer and Composite Electrolytes. Materials 14(14), 3840 (2021). 

    [5] Kasnatscheew, J.; Streipert, B.; Röser, S.; Wagner, R.; Cekic Laskovic, I.; Winter, M. Determining oxidative stability of battery electrolytes: validity of common electrochemical stability window (ESW) data and alternative strategies. Physical Chemistry Chemical Physics 19(24), 16078–16086 (2017). 

    [6] Gamry Instruments. Basics of Electrochemical Impedance Spectroscopy. Official application guide. Accessed November 19, 2026. 

    [7] Horner, J. S.; Whang, G.; Ashby, D. S.; Kolesnichenko, I. V.; Lambert, T. N.; Dunn, B. S.; Talin, A. A.; Roberts, S. A. Electrochemical Modeling of GITT Measurements for Improved Solid-State Diffusion Coefficient Evaluation. arXiv:2107.05835v2 (2021). Public author manuscript; journal DOI: 10.1021/acsaem.1c02218. 

    [8] NEWARE. Restore the graph to its original state with one click. Official BTSDA 8.0 tutorial, March 24, 2025. Accessed November 19, 2026.

    [9] NEWARE. Battery Research Solution. Official battery research solution. Accessed November 19, 2026. 

    [10] Wang, W.; Zhang, X.; Wang, X.; Gao, C.; Yin, J.; Wen, Q.; Wang, G. N/S Co-Doped Carbon-Coated Micro-Expanded Graphite for High-Performance Lithium-Ion Battery Anodes. Materials 18(11), 2477 (2025). DOI: 10.3390/ma18112477. 


    neware-battery-test-newareAI neware-battery-test-newareStore neware-battery-test-neware-newell

    A Complete Validation Solution

    Every piece of the puzzle, engineered to work in concert.

    View all

    Still can't find your answer?

    Our application engineers are ready to help with technical issues, calibration requests, and custom testing solutions.
    Name
    Country
    City Name
    Company Name
    Phone Number
    Email Address *
    Products
    Model
    Detailed Request
    NEWARE and Cookies
    We use cookies to personalize and improve your experience with our website. By continuing to browse the site you are agreeing to our use of cookies.