    EIS for Batteries From Measurement Principles to Data Analysis

    Electrochemical impedance spectroscopy (EIS) uses small electrical signals at different frequencies to examine how processes inside a battery respond to an external perturbation. It can reveal changes in impedance between operating states and, together with equivalent circuits, distribution of relaxation times analysis and data-driven models, provide information on resistance, characteristic times and battery health. This article starts with the measurement principles and explains how EIS data can be developed into results that support material evaluation, aging analysis and testing decisions.

    Latest updated: November 18, 2026 Reading time: 10 - 12 min

    1 Understanding EIS through a small perturbation

    A battery does not respond instantaneously to an applied current. Electron and ion conduction, interfacial charge accumulation, charge-transfer reactions and diffusion have different response times. EIS uses these differences by applying a small sinusoidal current or voltage around a defined operating point, varying the frequency and measuring the amplitude and phase of the response. High-frequency perturbations change rapidly, whereas low-frequency perturbations allow more time for the response to develop. Each process therefore contributes differently to the totalimpedance as frequency changes. [1]

    For current excitation, let the alternating current be ΔI(t) = Ia sin(ωt) and the corresponding alternating voltage be ΔV(t) = Va sin(ωt + φ). Here, ΔI and ΔV are the alternating components superimposed on the direct-current operating point; Iₐ and Vₐ are their amplitudes; φ is the voltage phase relative to the current; and ω = 2πf, with f in Hz. Complex impedance is defined as the ratio of the voltage and current phasors:

     

    Z′ and Z″ are the real and imaginary parts of impedance, both in Ω, and j is the imaginary unit. The amplitude ratio describes how much voltage response a current perturbation produces, while the phase difference describes their relative timing. Voltage and current are in phase for a pure resistor; capacitive or diffusion processes can introduce a phase shift. EIS therefore produces a set of complex impedance values that varies with frequency, rather than a single fixed internal resistance.

    EIS Small Signal Principle

    Figure 1. EIS amplitude and phase measurement and a two-electrode system

    Figure 1a illustrates this relationship using voltage excitation. The dashed blue line is the applied voltage and the solid red line is the current response. They have the same frequency but different amplitudes and peak times. The symbol φ0 in the figure denotes the voltage amplitude, corresponding to Va in this article. The amplitude ratio gives |Z|, and the time shift determines the phase difference. Repeating the measurement at different frequencies produces an impedance spectrum. Figure 1b depicts a planar two-electrode and electrolyte system to show how interfaces, the electrolyte and parasitic elements jointly affect the response; it is not a structural diagram of a lithium-ion full cell. [2]

    2 Reading impedance plots and equivalent circuits through frequency response

    Frequency reflects the response time of a process

    Different processes have different characteristic times. At high frequencies, each perturbation cycle is short, leaving less time for slow diffusion to develop. As frequency decreases, interfacial polarization and concentration changes become more apparent in the response. For an ideal resistor and capacitor connected in parallel, the characteristic time is τ = RC and the characteristic frequency is 1/(2πτ). A frequency sweep thus compares responses over different time scales; it does not isolate a single reaction at every frequency point. [1]

    A Nyquist plot shows Z′ on the horizontal axis and −Z″ on the vertical axis, with each point representing one measurement frequency. Capacitive responses generally lie above the horizontal axis and inductive responses below it. A Bode plot shows impedance magnitude |Z| and phase angle φ against frequency, making the frequency location of each feature explicit. Both plots represent the same data: the Nyquist plot makes intercepts and arcs easy to compare, while the Bode plot helps locate frequency ranges and examine phase changes.

    EIS Bode and Nyquist Comparison

    Figure 2. Bode and Nyquist plots of the same cell impedance spectrum

    Figure 2a is the Bode plot of a fully charged lithium-ion cell. Frequency is plotted on a logarithmic horizontal axis; the left vertical axis shows impedance magnitude |Z| in mΩ, and the right axis shows phase angle arg(Z) in degrees. Open circles and open diamonds are the measured magnitude and phase points, respectively, while the black and red solid lines are their corresponding fits. Locate a frequency first, then read the magnitude and phase from their respective vertical axes. [3]

    Figure 2b presents the same data as a Nyquist plot, with Re(Z) on the horizontal axis and −Im(Z) on the vertical axis, both in mΩ. The labels at 10 kHz, 1 kHz, 2.5 Hz and 0.01 Hz link positions on the curve to frequency. The positive phase at high frequencies in Figure 2a corresponds to the inductive response below the horizontal axis in Figure 2b. When the phase is negative, −Im(Z) is positive and the curve lies above that axis. Reading both plots together identifies the shape of a response and the frequency range in which it occurs. [3]

    Following battery processes from high to low frequency

    At the high-frequency end, examine the ohmic and inductive contributions first. Near 10 kHz in Figure 2, the Nyquist curve lies below the real axis and the Bode phase is positive. This indicates an inductive contribution, which may arise from conductors inside the cell, tabs and test leads. As frequency decreases and the curve approaches the real axis, a model can help estimate the series ohmic resistance RΩ. This includes contributions from ionic conduction through the electrolyte, current collectors and contacts. RΩ shifts the overall real component and is not present only at high frequencies. If other processes still contribute substantially, the real-axis crossing cannot simply be treated as a pure ohmic resistance. [1,3]

    Arcs at intermediate frequencies mainly reflect interfacial processes. In Figure 2, moving from approximately 1 kHz toward 2.5 Hz traces an arc that can be described by charge-transfer and double-layer responses. Charge-transfer resistance describes opposition to the interfacial reaction, while the double layer represents charge accumulation at the electrode–electrolyte interface. Resistance to lithium-ion transport through the solid electrolyte interphase (SEI), together with the film's capacitive response, may produce an additional arc, often on the relatively higher-frequency side. Film and charge-transfer processes can overlap, so a depressed arc need not represent just one reaction, and its entire width cannot automatically be assigned to charge-transfer resistance. [1,3]

    The low-frequency tail is associated with slower mass-transport processes. As frequency decreases from 2.5 Hz toward 0.01 Hz in Figure 2, the curve enters a tail extending upward and to the right. Longer time scales allow concentration changes in the electrolyte and active-material particles to contribute, often involving ion transport and solid-state diffusion. When ideal semi-infinite diffusion dominates, Warburg impedance appears as a line at approximately 45° in a Nyquist plot with equal axis scales. The Bode phase approaches −45°, and the magnitude increases as frequency decreases. Finite diffusion lengths, pore structure and lithium-storage effects can change the tail in real cells, so not every low-frequency response is a straight 45° line. [1,3]

    These frequencies describe Figure 2; they are not universal boundaries for all cells. Chemistry, temperature, state of charge (SOC) and aging can shift response times, and positive- and negative-electrode processes overlap in a full-cell spectrum. To assign a feature, examine how it changes with these conditions and validate the interpretation using three-electrode measurements or physical models. Locating a feature at high, intermediate or low frequency is a starting point for further analysis. [4]

    Equivalent circuits turn curves into comparable parameters

    Once the frequency ranges and curve features are understood, an equivalent circuit model (ECM) quantifies them using resistors, capacitors and other elements. Consider a simplified model without inductance or diffusion: a series ohmic resistance RΩ followed by a parallel branch containing resistance R and capacitance C. Its impedance is:

    Equation 02 Equivalent Circuit 

    In this ideal single-arc model, the capacitor branch has low impedance at high frequencies, and the left Nyquist intercept approaches RΩ. At low frequencies, the capacitor branch impedance rises and the right intercept approaches RΩ + R, so the semicircle diameter equals R. The Bode magnitude likewise changes from RΩ at high frequencies to RΩ + R at low frequencies, with a phase change through the transition. The arc-apex frequency fp and time constant τ satisfy:

    Equation 03 Time Constant and Peak Frequency

    The arc width therefore gives the resistance contribution, while its apex frequency indicates the response time. If R and fp can both be identified reliably, C can be calculated from Equation (3). Here, fp is the frequency of the imaginary-component extremum for a single RC arc; it cannot simply be replaced by the frequency of the phase extremum in the Bode plot of the complete circuit. Figure 2 also contains a high-frequency inductive region and a low-frequency tail. Fitting the full spectrum requires suitable inductive or diffusion elements rather than a single RC branch for every process. [1,3]

    Real electrodes often produce depressed arcs, so a constant phase element (CPE) is commonly used to describe non-ideal capacitive behavior. Its Q parameter is not generally a capacitance. It can be equated with, or converted to, a capacitance only under specific exponent and circuit conditions; a fitted Q value should not automatically be reported in F. [1]

    EIS RC and CPE Comparison

    Figure 3. Nyquist arcs for ideal RC and resistor–CPE parallel branches

    Figure 3 illustrates why real spectra often require a CPE. The red curve is the semicircle formed by a resistor in parallel with an ideal capacitor; replacing that capacitor with a CPE produces the depressed yellow arc. The figure shows only the parallel branch, without the series ohmic resistance RΩ introduced above, so its left endpoint is at the origin. Adding RΩ shifts the whole curve along the real axis. [3]

    A common CPE expression is ZCPE = 1/[Q(jω)n]. At n = 1, the element becomes an ideal capacitor and Q directly represents capacitance. For the common case 0 < n < 1, Q has units of S·sⁿ and the arc departs from an ideal semicircle. Select elements according to the spectrum: a depressed arc cannot be assigned to a single microscopic process from its shape alone, and a change in Q alone is not a reliable measure of a capacitance change. [1,3]

    Fitting usually treats the real and imaginary components together using complex nonlinear least squares, with parameter bounds and appropriate weighting. Plot the fitted model in both Nyquist and Bode form to check that it reproduces the arc shapes, magnitude and phase together. Then examine residuals versus frequency and parameter uncertainty. Adding elements can increase compensation between parameters, so start with the simplest structure that explains the main responses. The physical interpretation of its parameters still requires validation through changes in operating conditions or separate electrode measurements.

    3 Battery testing problems that EIS can address

    Comparing materials and interface designs

    When screening electrode materials, electrolytes, additives or interfacial coatings, EIS can compare impedance under the same SOC, temperature and test history. A smaller arc can motivate further investigation of lower interfacial polarization; a change in the low-frequency response can be examined with mass-transport models to assess diffusion or pore-transport effects. Electrode area, loading, compaction and electrolyte quantity also influence the result and must be controlled in a comparison.

    For example, when comparing two electrolyte formulations, record both the initial spectra and spectra at matched cycling stages to track the size and growth of the interfacial arcs. A formulation with lower initial impedance may not retain that advantage after cycling. Comparing impedance changes alongside capacity retention and rate performance helps distinguish an initial performance improvement from longer-term interfacial stability and supports further formulation screening.

    Tracking aging and investigating performance loss

    Capacity testing indicates how much charge a battery can still store, while EIS adds information about changes in its opposition to current flow. During cycling or calendar aging, periodically returning a cell to the same reference state makes it possible to track ohmic contributions, arcs and low-frequency features separately. These changes help narrow the focus of failure analysis and can be compared with rate performance, voltage drop under direct-current pulses and capacity fade. For example, two cell groups may have similar capacity retention but different increases in polarization impedance. Pulse or rate testing can then determine whether the larger increase is accompanied by reduced output capability. Relating impedance changes to cycling stages also helps identify when performance loss begins to accelerate and which operating conditions or material issues need further investigation.

    EIS Aging Spectra

    Figure 4. Evolution of cell impedance spectra during cycling at different charge rates

    Figure 4 provides an example of this approach. Its three panels correspond to charge rates of approximately 0.33 C, 1 C and 1.67 C. Cycling was performed at 25 °C over a 10–90% SOC window, while impedance checks were consistently conducted at 25 °C and 50% SOC. Color indicates cumulative equivalent full cycles (EFC), not the SOC at measurement. Each panel also overlays data from three cells, showing both the evolution with aging and differences between cells. [5]

    First compare positions near the high-frequency real-axis region, then examine changes in the arcs and low-frequency response. The panels use different horizontal-axis ranges, so apparent arc width on the page is not a direct measure of resistance. A rightward shift cannot immediately be attributed to growth of a particular interfacial film. A common reference state reduces temperature and SOC effects and provides comparable data for parameter fitting and mechanism validation.

    Providing inputs for state estimation and consistency screening

    For cells of the same model tested under the same conditions, EIS adds information beyond capacity and direct-current internal resistance when comparing cell consistency. Real and imaginary components at selected frequencies, or validated fitted parameters, can define a reference distribution for a batch. This helps identify cells that deviate substantially and the frequency ranges in which the differences occur. The results can guide repeat testing or further grouping; screening thresholds should reflect measurement repeatability and actual performance results.

    To estimate state of health (SOH), pair impedance features with measured capacity or other state indicators, establish a calibration relationship for that cell type and validate it using independent samples. Temperature, SOC and aging all affect impedance, so align SOC and temperature before comparing aging states. Useful outputs can include consistency rankings, a list of cells requiring repeat tests or validated SOH estimates. [3]

    4 DRT helps separate overlapping responses

    When several arcs overlap in a Nyquist plot, it can be difficult to decide how many RC branches to include. The distribution of relaxation times (DRT) represents a spectrum as contributions with different time constants. A common expression using an RC relaxation kernel and treating series inductance separately is:

    Equation 04 DRT Impedance Model

    Here, R∞ is the high-frequency ohmic term, L is the series inductance, τ is relaxation time and γ(lnτ) describes the impedance contribution per logarithmic time interval, with units of Ω in this formulation. With this normalization, integrating a resolved peak along the lnτ axis gives its resistance contribution, while the peak position reflects its characteristic time. Considering peak area, position and their changes with operating conditions is more informative for comparisons across stages than peak height alone. [6]

    EIS DRT Separation

    Figure 5. Overlapping responses in a simulated impedance spectrum and their DRT separation

    Figure 5 is a simulation based on a known circuit: an ohmic resistor in series with an RC branch and a ZARC branch, the latter representing the non-ideal relaxation of a resistor in parallel with a CPE. The two contributions overlap in the left Nyquist plot, making their number difficult to determine from the broad arc alone. The DRT on the right resolves two clearer peaks. Although the original legend uses the word “measurement,” these are not measured cell data, and the example does not establish that a real cell necessarily has two independent reactions. [7]

    The right-hand horizontal axis is log10(τ/s): positions farther to the right indicate longer characteristic times and lower characteristic frequencies. The upper axis shows the corresponding frequency scale. The vertical quantity hk uses the original paper's discrete resistance-contribution definition, which has a different normalization from the continuous distribution γ in Equation (4). Definitions must therefore be aligned before comparing software outputs. The gray regions show the individual decomposed peaks. The reconstructed curve on the left provides another check: the separated responses should reproduce the input spectrum. [7]

    DRT inversion is an ill-posed problem, and noise can be amplified into additional small peaks. Common approaches include Tikhonov regularization, non-negativity constraints, and Bayesian or Gaussian-process methods. These limit unstable solutions through smoothness constraints or probabilistic priors. Too little regularization may generate spurious peaks, while too much may merge neighboring peaks. Report the inversion settings, reconstructed spectrum and residuals, and check whether the main peaks remain stable as analysis settings change. [6]

    DRT reduces the need to specify a discrete circuit structure in advance, but still depends on the selected response kernel, constraints and frequency window. One peak can combine several processes, and one process can produce a broad distribution. Low-frequency diffusion and inductive responses also require suitable treatment. A peak's time range alone does not justify labeling it as SEI growth, lithium plating at the negative electrode or a positive-electrode reaction. Research using physical models has demonstrated clear limits to such one-to-one assignments. [4]

    5 Data-driven methods relate impedance features to battery state

    For capacity estimation or anomaly detection, inputs can include the real component, imaginary component, magnitude and phase at selected frequencies, parameters obtained from the equivalent circuit fitting discussed earlier, such as resistances and characteristic times, and DRT peak features. Alternatively, a regression model can learn the relationship between a complete spectrum and the target state. Dimensionality-reduction methods such as principal component analysis help compress features and examine sample distributions, while supervised methods such as Gaussian-process regression require corresponding capacity or lifetime labels.

    Zhang and colleagues combined EIS with Gaussian-process regression for capacity estimation and remaining useful life prediction in commercial lithium cobalt oxide/graphite cells. Figure 6 shows capacity-estimation results at 25 °C and the weights assigned to different impedance features. This demonstrates that EIS can provide useful inputs for state estimation. However, the study used the same charge and discharge rates for its training and test cells; transfer to other rates still requires validation. [8]

    EIS Capacity Estimation

    Figure 6. A research example of capacity estimation using EIS and Gaussian-process regression

    When developing a model, separate training and test data by cell so that adjacent cycles from the same cell do not appear in both sets and inflate apparent performance. Changes in temperature, SOC, chemistry and test equipment also require separate validation. Capacity-based SOH still requires capacity measurements for calibration, while remaining-life predictions also depend on future operating conditions. A numerical output alone does not establish that a model is suitable for a new product or operating regime.

    6 Validating the interpretation of processed results

    EIS can provide information at three levels. Direct measurements describe impedance, phase and their changes with frequency. Models provide ohmic contributions, polarization-related parameters, characteristic times and distributions. Independent calibration can then support estimates of capacity, SOH, anomaly categories or lifetime. The first two levels describe the battery's response; the third connects that response to a specific engineering objective. An analysis report should make clear which level its results represent.

    Consider an arc that grows after cycling. First confirm that temperature, SOC and rest history match between the earlier and later measurements, then check whether the high-frequency ohmic contribution has also changed. Use equivalent circuit fitting or DRT to locate the time scales responsible for the main change. If the associated polarization contribution continues to rise, pulse and rate tests can establish whether power capability is also declining. Assigning the change to a particular electrode or aging mechanism requires further evidence, such as three-electrode measurements or characterization after cell disassembly.

    7 Building a repeatable EIS testing workflow

    A practical workflow is to establish a reference state, measure the spectrum, check its quality, extract features and cross-validate the results. First define whether the objective is material comparison, aging analysis or state estimation. Then standardize SOC preparation, temperature, rest criteria and connections. The frequency range should cover the processes of interest while accounting for low-frequency measurement time and high-frequency parasitic effects; a wider range is not automatically better.

    Once a suitable spectrum is available, selected frequencies or clearly defined features can support rapid comparisons. Use equivalent circuit fitting when a small set of parameters needs to be tracked, and DRT when responses overlap strongly. State prediction requires sufficient calibration data. Retain the original spectra, processing rules, model versions and validation results so that later changes can be traced to the battery, the measurement or the analysis.

    8 Maintaining measurement conditions and linked data with NEWARE EIS systems

    Applying these methods throughout a study requires capacity, cycling history and impedance spectra to be linked to the same cell and reference state. The NEWARE CT-8002S-5V100mA-EIS battery testing system supports simultaneous EIS testing on two channels, with EIS included on each channel, and allows impedance measurements to be integrated with charge–discharge testing. For materials research and low-current cell testing, this arrangement supports repeated impedance measurements at different cycling stages while reducing changes caused by moving cells and reconnecting them.

    NEWARE EIS Battery Tester

    Figure 7. Official product image of the NEWARE CT-8002S-5V100mA-EIS testing system

    The official product page lists a voltage range of −5 V to 5 V, a maximum current of 100 mA, current ranges of 0.1, 1, 5, 10, 50 and 100 mA, and voltage and current accuracy of ±0.01% F.S. (full scale). Interpret these specifications in relation to the sample's voltage, current requirements and selected range. They are not equivalent to impedance-magnitude or phase accuracy across the full frequency range. Selection also requires checking EIS accuracy at the target impedance, excitation conditions, frequency coverage and connection configuration. The 1000 Hz value in Figure 7 is the data-recording rate, not a stated upper EIS sweep frequency. Likewise, a current conversion time measured in microseconds is not the time needed to acquire a complete spectrum.

    Matching excitation amplitude to cell impedance

    Before testing a specific cell, confirm the small-signal conditions. Classical EIS approximates the battery as a linear, time-invariant system around an operating point. Excessive excitation may introduce nonlinearity, while an amplitude that is too small can leave the response obscured by noise. Confirm a suitable amplitude through repeated measurements at different amplitudes. Potentiostatic EIS controls the alternating voltage and measures the alternating current; galvanostatic EIS controls the alternating current and measures the alternating voltage. The chosen method must match the excitation modes supported by the equipment. [1]

    For a low-impedance cell, a given voltage amplitude requires a larger alternating current, while a given current amplitude may produce only a very small voltage response. When using the 100 mA-class system described above, evaluate its actual EIS excitation capability, selected range and ability to resolve the voltage response against the sample impedance. The maximum charge–discharge current alone does not establish suitability. Confirm that the output is not overloaded and that the response can be resolved consistently before comparing spectra from different cycling stages.

    Allowing time for state stabilization and low-frequency measurements

    Low-frequency tests require time for cell stabilization and signal acquisition. One cycle at 0.01 Hz, for example, takes 100 s, and a complete measurement usually also requires settling time and sampling over several cycles. If cell temperature, SOC or open-circuit voltage continues to change during this period, the spectrum may include state drift. In cycling studies, allow the cell to rest at the agreed SOC and temperature, then begin EIS once consistent stability criteria are met. [1]

    Integrating charge–discharge testing with EIS helps maintain consistent sample connections and records. Distinguish EIS performed at rest between charge–discharge steps from online EIS during active charging or discharging. In the latter case, the operating point changes continuously, requiring suitable measurement methods and stability assessment; interpretations developed for a resting cell cannot simply be transferred unchanged.

    NEWARE EIS Analysis Interface

    Figure 8. NEWARE's official EIS interface showing impedance curves and frequency data

    After measurement, store each spectrum with its corresponding capacity, cycle count and temperature records. The EIS analysis interface in Figure 8 provides access to impedance curves and frequency data. Validated fitting, DRT or statistical analysis can then be applied according to the research objective. Consistent measurement conditions and complete original records are essential for relating the frequency-dependent changes discussed above to the actual state of the cell.

    References

    [1] Lazanas, A. C.; Prodromidis, M. I. Electrochemical Impedance Spectroscopy—A Tutorial. ACS Measurement Science Au 3(3), 162–193 (2023).https://doi.org/10.1021/acsmeasuresciau.2c00070

    [2] Abbas, Y.; van Smeden, L.; Verschueren, A. R. M.; Zevenbergen, M. A. G.; Oudenhoven, J. F. M. Modeling Electrochemical Impedance Spectroscopy Using Time-Dependent Finite Element Method. Sensors 24(22), 7264 (2024).https://doi.org/10.3390/s24227264

    [3] Jiang, S.; Song, Z. Estimating the State of Health of Lithium-Ion Batteries with a High Discharge Rate through Impedance. Energies 14(16), 4833 (2021).https://doi.org/10.3390/en14164833

    [4] Rüther, T.; Hileman, W.; Plett, G. L.; Trimboli, M. S.; Danzer, M. A. Demystifying the Distribution of Relaxation Times: A Simulation-Based Investigation into the Limits and Possibilities of Interpretation for Lithium-Ion Batteries. Journal of The Electrochemical Society 171(6), 060508 (2024).https://doi.org/10.1149/1945-7111/ad4fe5

    [5] Luh, M.; Blank, T. Comprehensive battery aging dataset: capacity and impedance fade measurements of a lithium-ion NMC/C-SiO cell. Scientific Data 11, 1004 (2024).https://doi.org/10.1038/s41597-024-03831-x

    [6] Ciucci, F.; Chen, C. Analysis of electrochemical impedance spectroscopy data using the distribution of relaxation times: A Bayesian and hierarchical Bayesian approach. Electrochimica Acta 167, 439–454 (2015).https://doi.org/10.1016/j.electacta.2015.03.123

    [7] Danzer, M. A. Generalized Distribution of Relaxation Times Analysis for the Characterization of Impedance Spectra. Batteries 5(3), 53 (2019).https://doi.org/10.3390/batteries5030053

    [8] Zhang, Y.; Tang, Q.; Zhang, Y.; Wang, J.; Stimming, U.; Lee, A. A. Identifying degradation patterns of lithium ion batteries from impedance spectroscopy using machine learning. Nature Communications 11, 1706 (2020).https://doi.org/10.1038/s41467-020-15235-7


    neware-battery-test-newareAI neware-battery-test-newareStore neware-battery-test-neware-newell

    A Complete Validation Solution

    Every piece of the puzzle, engineered to work in concert.

    View all

    Still can't find your answer?

    Our application engineers are ready to help with technical issues, calibration requests, and custom testing solutions.
    Name
    Country
    City Name
    Company Name
    Phone Number
    Email Address *
    Products
    Model
    Detailed Request
    NEWARE and Cookies
    We use cookies to personalize and improve your experience with our website. By continuing to browse the site you are agreeing to our use of cookies.